https://www.avient.com/resource-center/services/cycleworks-innovation-center-plastic-recycling
Screens and evaluates additive and colorant systems in the recycling process
ColorMatrix™ Optica™ Toners & Colors for Enhanced Recyclability
https://www.avient.com/products/polymer-additives/processing-enhancement-additives/cesa-plastone-processing-enhancing-additive
Color and Additives Solutions Overview
Colorant and additives overview and capabilities
https://www.avient.com/news/sustainable-tpes-avient-featured-spe-tpo-conference
This includes technologies for lightweighting, colorants for secondary paint replacement, and bio-polymers.
Experts from Avient will be on hand at booth #24 throughout the conference to help customers better understand novel sustainable performance materials, including specialized polymer colorants, functional additives, and engineered material formulations.
https://www.avient.com/news/polyone-presents-leading-edge-solutions-fakuma-2015
Ranging from colorants and additives to engineered polymer formulations, these solutions can help customers operate more efficiently and design better.
PolyOne is also announcing the availability of the reSound™ NF Natural Fiber Reinforced Composites in brilliant colors and extrusion formulations, making the material more useful for building & construction, sporting goods and other applications.
https://www.avient.com/idea/taking-guesswork-out-laser-marking
The beam changes the molecular structure of the additive, causing a color change that results in a permanent marking.
Sourcing the additive as a masterbatch, often bundled with colorant, makes it easier to add to your production process.
https://www.avient.com/sites/default/files/2023-01/Mevopur Healthcare Colorants and Formulations Special Effects Application Bulletin_0.pdf
Mevopur™ Healthcare Colorants and Formulations
Special Effect Colorants for Healthcare Devices and
Pharmaceutical Packaging
Self-administered medication, for example via
pen devices and inhalers, has been the norm for
many years.
Ingredients used in the
Mevopur™ portfolio have been tested to industry
standards that support applications in both
medical devices and pharmaceutical packaging.*
KEY CHARACTERISTICS
• Manufactured at four ISO 13485 certified
manufacturing sites, providing global
consistency and increased security of supply
• Documented change control beyond CAS
number, reducing risk of change
• Non-phthalate and formulated without
animal-derived substances
• Available as pre-colored formulation or
concentrate and for use in different polymers
REGULATORY SUPPORT
• Raw materials tested to:
- ISO 10993-1 and USP biological
evaluation
- European Pharmacopeia 3.1.3/3.1.5
(polyolefin)
- USP (polyethylene)
- ICH Q3D elemental impurities
• Registered Drug Master File (Type III) and/or
Device Master File
• Food contact established with FDA/EU**
APPLICATION BULLETIN
* Design note: Effect colors require careful consideration of part design and
polymer flow paths to minimize visible flow lines.
https://www.avient.com/resources/safety-data-sheets?page=6686
5030-FT-72 PA 6 NAT
19718 COLOR MB X07670 V3
PP FR 8-6 LMS-1000
https://www.avient.com/resources/safety-data-sheets?page=210
PEBBLE FLAIR 6
COLOR SPA PINK PEARL
PP FR 8-6 LMS-1000
https://www.avient.com/resources/safety-data-sheets?page=5833
506756JPMB WHITE
MC-72970ST HIPS WHITE Q520-6-3 849334
PP FR 8-6 LMS-1000
https://www.avient.com/sites/default/files/2024-03/Nymax _ Nymax REC Processing Guide.pdf
Degraded/
overheated
material
• Decrease melt temperature
• Decrease back pressure
• Use smaller barrel
• Decrease injection speed
Gate location
and/or size
• Relocate gate to nonstress area
• Increase gate size to allow higher flow rate
and lower molded in stress
Fibers/Minerals on
Surface or Uneven
Surface Appearance
Melt temperature
too low
• Increase melt temperature
• Increase mold temperature
• Increase injection speed
Insufficient packing • Increase hold pressure and time• Increase shot size
Processing Guide 5
Problem Cause Solution
Sink Marks
Part geometry
too thick
• Reduce wall thickness
• Reduce rib thickness
Melt too hot • Decrease nozzle and barrel temperatures• Decrease mold temperature
Insufficient
material volume
• Increase shot size
• Increase injection rate
• Increase packing pressure
• Increase gate size
Flash
Injection pressure
too high
• Decrease injection pressure
• Increase clamp pressure
• Decrease injection rate
• Increase transfer position
Excess
material volume
• Adjust transfer position
• Decrease pack pressure
• Decrease shot size
• Decrease injection rate
Melt and/or mold
too hot
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
• Decrease screw speed
Loose clamp • Reset mold height• Increase clamp tonnage
Shrink
Too much
shrink
• Increase cooling time
• Decrease mold temperature
Too little
shrink
• Decrease cooling time
• Increase mold temperature
Troubleshooting Recommendations
6 Nymax Polymer Formulations
Troubleshooting Recommendations
Problem Cause Solution
Burning
Process related
• Decrease nozzle and barrel temperatures
• Decrease mold temperature
• Decrease injection rate
Mold design • Clean, widen and increase number of vents• Increase gate size to reduce shear
Wet material
• Check moisture.